material

AlN

ID:

mp-661


Tags: Aluminium nitride - 2H Aluminum nitride Aluminium nitride - wurtzite-type Aluminium nitride

Material Details

Final Magnetic Moment
0.000 μB

Calculated total magnetic moment for the unit cell within the magnetic ordering provided (see below). Typically accurate to the second digit.

Magnetic Ordering
NM
Formation Energy / Atom
-1.595 eV

Calculated formation energy from the elements normalized to per atom in the unit cell.

Energy Above Hull / Atom
0.000 eV

The energy of decomposition of this material into the set of most stable materials at this chemical composition, in eV/atom. Stability is tested against all potential chemical combinations that result in the material's composition. For example, a Co2O3 structure would be tested for decomposition against other Co2O3 structures, against Co and O2 mixtures, and against CoO and O2 mixtures.

Density
3.20 g/cm3

The calculated bulk crystalline density, typically underestimated due calculated cell volumes overestimated on average by 3% (+/- 6%)

Decomposes To
Stable
Band Gap
4.054 eV

In general, band gaps computed with common exchange-correlation functionals such as the LDA and GGA are severely underestimated. Typically the disagreement is reported to be ~50% in the literature. Some internal testing by the Materials Project supports these statements; typically, we find that band gaps are underestimated by ~40%. We additionally find that several known insulators are predicted to be metallic.

Space Group

Hermann Mauguin
P63mc [186]
Hall
P 6c 2c
Point Group
6mm
Crystal System
hexagonal

Electronic Structure

Topological data for ICSD ID 31169 from Topological Materials Database
Topological Classification
trivial*
Subclassification
LCEBR
* trivial insulator or metal
Linear Combination of Elementary Band Representations
Band Structure
Density of States
Warning! Semi-local DFT tends to severely underestimate bandgaps. Please see the wiki for more info.

sign indicates spin ↑ ↓

Vibrational Properties

Reference for phonon calculations and visualization: Visualize with phononwebsite

Phonon dispersion

Density of States
Warning! These calculations were performed using a PBEsol exchange correlation functional in the framework of DFPT using the Abinit code. Please see the wiki for more info.

X-Ray Diffraction

    Select radiation source:
  • Cu
  • Ag
  • Mo
  • Fe

Calculated powder diffraction pattern; note that peak spacings may be affected due to inaccuracies in calculated cell volume, which is typically overestimated on average by 3% (+/- 6%)

X-Ray Absorption Spectra

FEFF XANES

Select an element to display a spectrum averaged over all sites of that element in the structure.

Apply Gaussian smoothing:

0 eV
3 eV
FWHM: 0 eV

Download spectra for every symmetrically equivalent absorption site in the structure.

Download FEFF Input parameters.

Warning: These results are intended to be semi-quantitative in that corrections, such as edge shifts and Debye-Waller damping, have not been included.

Substrates

Reference for minimal coincident interface area (MCIA) and elastic energy:
substrate orientation:
substrate material substrate orientation film orientation elastic energy [meV] MCIA [Å2]
InSb (mp-20012) <1 1 1> <0 0 1> 0.001 76.3
CdTe (mp-406) <1 1 1> <0 0 1> 0.004 76.3
CdS (mp-672) <1 0 0> <1 0 0> 0.006 172.7
LaAlO3 (mp-2920) <0 0 1> <0 0 1> 0.006 25.4
KCl (mp-23193) <1 1 1> <0 0 1> 0.007 211.9
SiO2 (mp-6930) <1 0 1> <1 0 0> 0.011 141.3
Au (mp-81) <1 1 1> <0 0 1> 0.017 211.9
Al (mp-134) <1 0 0> <1 0 1> 0.020 196.2
LiAlO2 (mp-3427) <1 0 0> <1 1 1> 0.024 199.3
LaF3 (mp-905) <0 0 1> <0 0 1> 0.029 135.6
YAlO3 (mp-3792) <0 0 1> <0 0 1> 0.037 84.8
ZrO2 (mp-2858) <1 0 1> <1 1 1> 0.039 85.4
GaTe (mp-542812) <1 0 0> <0 0 1> 0.040 135.6
CdWO4 (mp-19387) <0 0 1> <1 0 1> 0.043 214.1
PbSe (mp-2201) <1 0 0> <0 0 1> 0.044 271.3
MoSe2 (mp-1634) <1 0 1> <1 0 0> 0.045 157.0
InAs (mp-20305) <1 1 1> <0 0 1> 0.046 262.8
GaSb (mp-1156) <1 0 0> <0 0 1> 0.046 271.3
KTaO3 (mp-3614) <1 0 0> <1 0 1> 0.048 196.2
LaAlO3 (mp-2920) <1 0 1> <0 0 1> 0.052 76.3
LiAlO2 (mp-3427) <1 0 1> <1 0 0> 0.055 172.7
CdSe (mp-2691) <1 0 0> <0 0 1> 0.056 271.3
LaAlO3 (mp-2920) <1 1 1> <0 0 1> 0.058 127.2
DyScO3 (mp-31120) <0 1 0> <1 1 0> 0.059 217.5
ZnTe (mp-2176) <1 1 1> <0 0 1> 0.061 262.8
GdScO3 (mp-5690) <1 1 1> <1 1 1> 0.063 142.4
ZnSe (mp-1190) <1 0 0> <1 0 1> 0.065 196.2
WSe2 (mp-1821) <1 1 1> <0 0 1> 0.069 262.8
DyScO3 (mp-31120) <0 0 1> <1 0 1> 0.072 124.9
Ag (mp-124) <1 1 1> <0 0 1> 0.078 211.9
CaCO3 (mp-3953) <1 0 0> <1 0 0> 0.083 172.7
NaCl (mp-22862) <1 0 0> <1 0 1> 0.086 196.2
YAlO3 (mp-3792) <1 0 1> <1 1 0> 0.088 244.7
Al2O3 (mp-1143) <0 0 1> <0 0 1> 0.100 59.3
TiO2 (mp-2657) <1 0 0> <1 0 0> 0.103 109.9
GaAs (mp-2534) <1 0 0> <1 0 1> 0.106 196.2
InP (mp-20351) <1 1 0> <1 1 1> 0.107 199.3
TbScO3 (mp-31119) <0 1 0> <1 1 0> 0.119 217.5
MgF2 (mp-1249) <0 0 1> <0 0 1> 0.122 178.0
SiC (mp-7631) <1 0 1> <0 0 1> 0.127 144.1
TbScO3 (mp-31119) <0 0 1> <1 0 1> 0.132 124.9
ZrO2 (mp-2858) <1 0 0> <0 0 1> 0.135 84.8
C (mp-66) <1 1 0> <1 1 0> 0.153 54.4
Ni (mp-23) <1 1 1> <1 0 0> 0.154 172.7
SiC (mp-7631) <1 1 1> <0 0 1> 0.167 245.8
SiC (mp-8062) <1 1 0> <0 0 1> 0.171 135.6
SiC (mp-7631) <1 1 0> <1 1 0> 0.175 81.6
LiGaO2 (mp-5854) <1 1 1> <0 0 1> 0.175 169.5
SiC (mp-7631) <1 0 0> <1 0 0> 0.175 47.1
ZnTe (mp-2176) <1 1 0> <0 0 1> 0.176 271.3
Up to 50 entries displayed.
minimal coincident interface area.

Elasticity

Reference for tensor and properties:
Stiffness Tensor Cij (GPa)
376 129 98 0 0 0
129 376 98 0 0 0
98 98 353 0 0 0
0 0 0 113 0 0
0 0 0 0 113 0
0 0 0 0 0 124
Compliance Tensor Sij (10-12Pa-1)
3.1 -0.9 -0.6 0 0 0
-0.9 3.1 -0.6 0 0 0
-0.6 -0.6 3.2 0 0 0
0 0 0 8.9 0 0
0 0 0 0 8.9 0
0 0 0 0 0 8.1
Shear Modulus GV
122 GPa
Bulk Modulus KV
195 GPa
Shear Modulus GR
121 GPa
Bulk Modulus KR
194 GPa
Shear Modulus GVRH
122 GPa
Bulk Modulus KVRH
194 GPa
Elastic Anisotropy
0.03
Poisson's Ratio
0.24

Piezoelectricity

Reference for tensor and properties: Methodology
Piezoelectric Tensor eij (C/m2)
0.00000 0.00000 0.00000 0.00000 -0.28930 0.00000
0.00000 0.00000 0.00000 -0.28931 0.00000 0.00000
-0.58006 -0.58006 1.46115 0.00000 0.00000 0.00000
Piezoelectric Modulus ‖eijmax
1.67568 C/m2
Crystallographic Direction vmax
0.00000
-0.00000
-1.00000

Dielectric Properties

Reference for tensor and properties: Methodology
Dielectric Tensor εij (electronic contribution)
4.47 0.00 0.00
0.00 4.47 0.00
0.00 0.00 4.69
Dielectric Tensor εij (total)
8.23 0.00 0.00
0.00 8.23 0.00
0.00 0.00 9.74
Polycrystalline dielectric constant εpoly
(electronic contribution)
4.54
Polycrystalline dielectric constant εpoly
(total)
8.73
Refractive Index n
2.13
Potentially ferroelectric?
Unknown

Equations of State

Reference:
Equation E0 (eV) V0 (Å3) B C
mie_gruneisen -7.445 10.638 10.826 4.792
pack_evans_james -7.445 10.638 1.200 2.934
vinet -7.446 10.634 10.969 4.468
tait -7.446 10.631 1.215 5.052
birch_euler -7.445 10.637 1.357 -0.060
pourier_tarantola -7.447 10.633 0.205 1.971
birch_lagrange -7.452 10.636 0.755 5.708
murnaghan -7.444 10.647 1.176 2.829
Equations reference

Similar Structures beta feature

Explanation of dissimilarity measure: Documentation.
material dissimilarity Ehull # of elements
BeSiN2 (mp-7913) 0.1355 0.000 3
LiInSe2 (mp-20310) 0.1618 0.001 3
MgSnN2 (mp-1029791) 0.0638 0.000 3
ZnSnN2 (mp-1029469) 0.1275 0.000 3
Zn2SbN3 (mp-1029334) 0.1574 0.000 3
LiCo7O7F (mp-764039) 0.2216 0.052 4
LiCo5O5F (mp-764225) 0.2532 0.061 4
Li4VGa3O8 (mp-772233) 0.2862 0.038 4
Li2ZnSnS4 (mp-555186) 0.2212 0.000 4
ZnGaNO (mp-558481) 0.2637 0.059 4
CuH (mp-24093) 0.0369 0.062 2
MnS (mp-2562) 0.0484 0.018 2
CoO (mp-561373) 0.0330 0.007 2
CoO (mp-19128) 0.0345 0.007 2
AgH (mp-1096804) 0.0369 0.132 2
Ge (mp-1007760) 0.1727 0.020 1
Si (mp-165) 0.1794 0.011 1
C (mp-611426) 0.3325 0.145 1
C (mp-47) 0.1854 0.160 1
Ge (mp-1091415) 0.3368 0.022 1
Up to 5 similar elemental, binary, ternary, quaternary, etc. structures displayed (dissimilarity threshold 0.75). Ehull: energy above hull per atom [eV].

Synthesis Descriptions

The Sm, Y and Ca anhydrous nitrates were mixed with the AlN powder in ethanol and then decomposed into the Sm2O3-Y2O3-CaO sintering additives via calcining. Low-temperature sintering of the AlN cerami [...]
The FePt/AlN layered structures were deposited by a DC magnetron sputtering method onto fused quartz substrates at room temperature. The sputtering chamber pressure was reduced below 5105 Pa befor [...]
chef hat mixing beaker

Explore more synthesis descriptions for materials of composition AlN.

Text computed by synthesisproject.org.

Calculation Summary

Elasticity

Methodology

Structure Optimization

Run Type
GGA
Energy Cutoff
520 eV
# of K-points
None
U Values
--
Pseudopotentials
VASP PAW: Al N
Final Energy/Atom
-7.4449 eV
Corrected Energy
-29.7797 eV
-29.7797 eV = -29.7797 eV (uncorrected energy)

Detailed input parameters and outputs for all calculations


Show JSON History Show BibTex Citation Download BibTex Citation
ICSD IDs
  • 608626
  • 608627
  • 602460
  • 190420
  • 44107
  • 54697
  • 161881
  • 82790
  • 602459
  • 191772
  • 183638
  • 185441
  • 42001
  • 34475
  • 44106
  • 608624
  • 41480
  • 163953
  • 31169
  • 181362
  • 34236
  • 41482
  • 67767
  • 41542
Submitted by
User remarks:
  • Aluminium nitride

Displaying lattice parameters for primitive cell; note that calculated cell volumes are typically overestimated on average by 3% (+/- 6%). Note the primitive cell may appear less symmetric than the conventional cell representation (see "Structure Type" selector below the 3d structure)